Galvanized vs galvalume steel coil: which should you specify?

Galvanized and galvalume look almost identical and both carry a coating weight number, which is exactly why they get specified interchangeably by mistake. They are not interchangeable. GI is pure zinc and protects sacrificially. GL is an aluminium-zinc-silicon alloy that protects by barrier. The number 275 on a galvanized sheet and 150 on a galvalume sheet describe comparable films, not comparable mass — and that distinction is the key to choosing correctly.

The difference is the metallurgy, not the label

Hot-dip galvanized steel (GI) carries a coating of essentially pure zinc. Galvalume (GL, also sold as aluzinc) carries an alloy of about 55% aluminium, 43.4% zinc and 1.6% silicon, patented by BIEC International. The two protect steel by different mechanisms, and understanding that is what makes the specification decision straightforward.

Zinc protects sacrificially: it corrodes preferentially to the steel underneath, so a scratch heals itself as long as zinc remains nearby. Aluminium in galvalume forms a dense, passive oxide layer that acts as a barrier against oxygen and moisture, while the zinc fraction still provides sacrificial protection at cut edges and scratches. The alloy also develops a fine dendritic structure that hardens the surface, which is why galvalume resists transit abrasion better than soft zinc.

GI against GL, property by property

PropertyGalvanized (GI)Galvalume (GL)
Coating composition99% zinc55% Al / 43.4% Zn / 1.6% Si
Typical designationG90 / Z275AZ150
Coating weight (total, both sides)275 g/m²150 g/m²
Protection mechanismSacrificial — zinc corrodes in preference to steelBarrier — aluminium oxide blocks oxygen and moisture, zinc protects cut edges
Neutral salt spray to red rust (ASTM B117)300–500 hours at Z2751000–1500 hours at AZ150
Service life, inland / general construction15–25 years30–50 years
Solar reflectance (SRI)Low — about 0.35, absorbs heatHigh — above 0.75, reflects heat
Cut-edge behaviourZinc continues to protect the exposed edgeAluminium is less sacrificial; edges should still be sealed
Surface hardnessSoft, around 60–80 HVHarder, around 100–140 HV, resists transit abrasion
FormabilityExcellent — bends without crackingGood — care needed in tight bends
Relative material costBaselineTypically 10–20% higher
Typical applicationsIndustrial buildings, HVAC ducting, enclosures, general constructionPremium roofing, wall cladding, long-exposure outdoor use, coastal projects

Why Z275 and AZ150 are not comparable numbers

This is the point where most specifications go wrong. A buyer sees Z275 on a galvanized sheet and AZ150 on a galvalume sheet and concludes the galvanized one is heavier and therefore better. It is not a like-for-like comparison, because the numbers describe mass and the two alloys have very different densities.

Zinc has a density of about 7.14 g/cm³. The aluminium-zinc alloy in galvalume is roughly 3.0 g/cm³ — less than half. So an AZ150 coating, despite being 45% lighter by mass, delivers a physical film thickness comparable to a Z275 zinc coating. On equal film thickness, AZ150 gives two to four times the time to first red rust, and roughly double the service life in coastal and industrial atmospheres.

The practical rule: when comparing GI against GL, compare the film thickness and the environment, not the coating weight number. In dry inland conditions the gap narrows considerably and galvanized GI remains the more economical choice.

Which one to specify

Use galvalume AZ150 where the project is coastal, humid, tropical or industrial, or where the design life is long. Use galvanized GI where the environment is dry inland, the budget is tight, or the design life is shorter. There are specific exclusions worth knowing: galvalume should not be used in direct contact with copper or with wet green timber, and it performs poorly in high-ammonia environments such as livestock buildings, where galvanized GI is actually the better choice.

For pre-painted product, the base substrate makes a further difference. PPGI uses a galvanized base and PPGL uses a galvalume base. For exterior roofing, a PPGGL with a PVDF top coat on an AZ150 base is the longest-life combination available in this product family; for interior appliance applications where cost matters more than exposure life, PPGI on a Z120 base is the standard specification.

Storage, white rust and handling

Both coatings can develop surface staining if they are stored badly, and it is worth separating a storage problem from a material defect before rejecting a shipment. White rust on galvanized material is zinc oxide forming where condensation has been trapped between coil wraps. On galvalume the equivalent appears as dark spotting. In both cases the cause is the same: moisture trapped in an unventilated bundle.

Prevention is straightforward and worth specifying at order stage. Keep coils in a ventilated dry warehouse, never stack wet coils, and request VCI or oiled wrapping where the goods will be stored or transited through humid conditions. Anti-fingerprint coating is available for galvalume and is worth adding when the coil will be slitted or roll-formed downstream. Confirm the surface treatment on the order — chromated, anti-fingerprint or oiled — based on the humidity the material will actually see.

Frequently asked questions

Is AZ150 really better than Z275?

It depends on the environment, and you should not compare the two numbers directly because they express different things. Z275 means 275 g/m² of zinc; AZ150 means 150 g/m² of an aluminium-zinc alloy. Because the alloy is roughly half the density of zinc, an AZ150 coating delivers a comparable physical film thickness to a Z275 zinc coating. On that like-for-like basis AZ150 gives two to four times the time to red rust, and roughly double the service life in coastal and industrial atmospheres. In dry inland conditions the gap narrows considerably and GI is often the more economical choice.

Which is better for metal roofing?

For coastal, humid, or industrial roofing, galvalume AZ150 is the better specification — it reflects more solar heat, which lowers roof temperature and cooling cost in tropical climates, and it resists corrosion roughly twice as long. For dry inland projects with a shorter design life, galvanized Z120 or Z180 is usually sufficient and costs less. Galvalume is also the standard choice in markets such as Australia and the Gulf where coastal exposure is common.

Does galvalume need painting?

Not for corrosion protection — the alloy coating is designed to be left exposed and will outlast paint on a galvanized substrate in the same environment. It does need painting if a specific colour is required, in which case the paint system should be specified for an Al-Zn substrate rather than a zinc one. Note also that galvalume should not be used in direct contact with copper or in high-ammonia environments such as livestock buildings.

What is white rust and how do I prevent it?

White rust is zinc oxide forming on the coil surface when galvanized material is stored wet or with condensation trapped between wraps. It is a storage problem, not a material defect. Prevention is straightforward: keep coils in a ventilated dry warehouse, avoid stacking wet coils, and specify VCI or oiled wrapping for long storage or transit through humid climates. Chromate-free passivation is available and further reduces staining risk.

Can galvanized and galvalume be used together in one project?

They can, but you should be aware of galvanic coupling when the two metals are in direct contact. Galvalume has a more noble potential than galvanized steel, so where galvalume is attached to bare galvanized steel in a wet environment, the galvanized side corrodes preferentially. In practice this is managed by isolating the two materials, and in roof and wall assemblies the fasteners and flashings are usually the galvanically sacrificial element anyway.

Need help specifying your material?

Send grade, thickness, width, coating and quantity. We confirm mill availability and return a proforma with the applicable standard and delivery window — normally within one business day.

Request a Quote