Buyers who write "G90" in a purchase order usually know the answer they want. The problem is that G and Z designations are frequently confused, and a 25% difference in zinc coating weight is the difference between a roof that lasts 12 years and one that lasts 25. This guide sets out exactly what each grade means, how to convert between systems, and which environments each grade is actually suitable for.
Both systems describe the same thing — the total zinc coating weight on both faces of the coil — but they express it in different units and sit under different standards.
G is the ASTM A653 system, quoted in ounces per square foot (total, both sides). Z is the EN 10346 system, quoted in grams per square metre (total, both sides). The conversion is 1 oz/ft² ≈ 305 g/m², so the two describe the same coating once you translate the unit.
One point catches people out: the number is a total across both sides, not a per-side figure. A coil quoted as G90 / Z275 carries 275 g/m² in total, so 137.5 g/m² on each face. If you need a guaranteed minimum on a specific face, you have to say so explicitly on the order — because the mill is otherwise free to distribute the coating slightly unevenly between the two faces.
Coating weight is a mass. Coating thickness is what actually resists corrosion, and it is what a fabricator thinks in. The conversion comes from the density of zinc at 7.14 g/cm³:
Worked through for G90 / Z275: 275 ÷ 2 = 137.5 g/m² per side, and 137.5 × 0.14 = 19.3 µm per side. For G60 / Z180 the same calculation gives 90 × 0.14 = 12.6 µm per side. That is roughly a 53% difference in film thickness, which is why the corrosion life gap is so much wider than the numbers suggest.
Coating weight on both sides, equivalent single-side thickness, and the ASTM and EN designations that map to each other:
| Coating weight (g/m², both sides) | Thickness per side (µm) | ASTM A653 | EN 10346 | Salt spray to red rust | Typical environment |
|---|---|---|---|---|---|
| 60 | 4.2 | G30 | Z060 | 200–400 | Indoor, dry, warehouse, appliance housings |
| 80 | 5.6 | — | Z080 | 300–500 | Dry inland, light framing, interior use |
| 100 | 7.0 | G40 | Z100 | 400–600 | Indoor and sheltered, HVAC ducting |
| 120 | 8.4 | — | Z120 | 500–700 | Mild inland, sheds, fencing |
| 140 | 9.8 | G50 | Z140 | 600–1000 | Moderate humidity, industrial areas |
| 180 | 12.6 | G60 | Z180 | 1000–1500 | High-humidity coastal, chemical plant surrounds |
| 275 | 19.3 | G90 | Z275 | 1500–2500 | Marine, heavy industrial, salt spray regions |
| 350 | 24.5 | G115 | Z350 | 2000–3000 | Severe coastal, offshore, chemical processing |
| 450 | 31.5 | G140–G165 | Z450 | 2500–4000 | Offshore platforms, extreme industrial exposure |
| 600 | 42.0 | G185–G210 | Z600 | 3500–5000 | Marine splash zone, high-chloride industrial sites |
Salt spray figures are ASTM B117 neutral salt spray hours to first red rust. Treat them as a relative ranking between coatings rather than a prediction of field life — real performance depends on the environment and on whether the coating is intact when it is installed.
The right way to select a coating weight is to classify the site first and let the environment choose the grade. ISO 9223 does this with five corrosivity categories, from C1 very dry indoor to C5 marine and offshore.
| ISO 9223 category | Environment | Corrosivity | Zinc loss rate | Typical specification | Where it is used |
|---|---|---|---|---|---|
| C1 | Dry indoor | Very low | — | G30–G40 / Z060–Z100 | Interiors, air-conditioned buildings |
| C2 | Rural / urban inland | Low | — | G60–G90 / Z180–Z275 | Sheds, farm buildings, wall cladding |
| C3 | Urban / moderately humid | Medium | 0.2–0.6 µm/yr | G90–G115 / Z275–Z350 | Commercial buildings, industrial roofing |
| C4 | Coastal, industrial, urban traffic | High | 0.6–1.5 µm/yr | G115–G185 / Z350–Z600 | Coastal structures, chemical plants |
| C5 | Marine, offshore, high salinity | Very high | 1.5–3.0 µm/yr | G185+ / Z600 or higher | Offshore platforms, marine terminals |
G60 / Z180 and G90 / Z275 are the two grades you will be asked to compare most often, and the decision usually comes down to exposure and design life rather than price alone.
| Property | G60 / Z180 | G90 / Z275 |
|---|---|---|
| Coating weight, both sides | 180 g/m² | 275 g/m² |
| Thickness per side | 12.6 µm | 19.3 µm |
| Relative zinc mass | Baseline | 53% more |
| Neutral salt spray to red rust | 1000–1500 hours | 1500–2500 hours |
| ISO 9223 category suited to | C2, some C3 | C3, some C4 |
| Typical service life | 10–20 years | 20–35 years |
| Forming and welding | Simpler — softer zinc, less burn-through risk | Needs more care — thicker zinc needs controlled welding current and edge sealing |
| Best suited to | Interior framing, HVAC ducting, sheltered cladding, sheds | Standard roofing, wall cladding, purlins, C and Z sections, industrial buildings |
If in doubt, G90 / Z275 is the default for general outdoor construction — it is the most widely specified coating weight in the world for a reason. Step up to G115 or higher only where the environment genuinely demands it, because the thicker zinc does affect forming behaviour, welding procedure and cut-edge sealing requirements.
A specification line that removes all ambiguity looks like this:
Three details in that line are worth keeping. First, "minimum 275 g/m² total on both sides" removes the ±10% tolerance ambiguity that ASTM A653 permits on delivered weight. Second, non-spangled matters if the coil is to be painted or roll-formed, because the zinc crystal pattern will otherwise telegraph through the finish. Third, always specify the coil weight and inner diameter to match the buyer's uncoiler — it is the single most effective way to avoid a coil that arrives and cannot be processed.
Yes. G90 is the ASTM A653 designation (0.90 oz/ft² total on both sides) and Z275 is the equivalent EN 10346 designation (275 g/m² total). Both describe the same coating mass on the same product. You will see both on the same specification sheet depending on which standard the mill quotes against.
Thickness in microns per side equals the per-side coating weight in g/m² multiplied by 0.14. The constant comes from the density of zinc at 7.14 g/cm³. Since coating weight is always quoted as a total across both sides, divide by two first. So G90 (275 g/m² total) is 137.5 g/m² per side, which works out to about 19.3 microns per side.
G90 carries 275 g/m² against G60 at 180 g/m², so 53% more zinc by mass. On the converted per-side film thickness that is 19.3 microns against 12.6 microns. The practical effect is a materially longer time to first red rust — typically 1500–2500 hours in neutral salt spray for G90 against 1000–1500 hours for G60.
For a coastal site more than a few hundred metres from the shoreline, G90 (Z275) is the usual specification and performs well. Within direct marine exposure or salt spray, specify G185 (Z600) or a pre-painted system with a PVDF top coat, and seal cut edges with zinc-rich paint after fabrication. If the project is genuinely marine, discuss a zinc-aluminium-magnesium (ZAM) coating with the mill instead.
ASTM A653 permits a tolerance of ±10% on the total coating weight as delivered. This is worth knowing if you are specifying a minimum: always state the minimum total coating weight on both sides rather than relying on the nominal value, and check the actual figure on the mill test certificate when the shipment is weighed.
Yes, and it is frequently supplied passivated and oiled specifically so it can be painted or roll-formed downstream. Specify passivation and oil if the coil is going into a paint line, and confirm the passivation type — chrome-free is now the norm for European-bound material.
Send grade, thickness, width, coating and quantity. We confirm mill availability and return a proforma with the applicable standard and delivery window — normally within one business day.